| 烧结汝铁硼产品性能参数 | |||||||||||
| Product performance parameters of Sintered NdFeB | |||||||||||
| 性能 牌号 | 剩磁 | 矫顽力 | 内禀矫顽力 | 最大磁能积 | 工作温度 | ||||||
| KGs | kOe | kA/m | kOe | kA/m | MGOe | KJ/M3 | ℃ | ||||
| 最小值 | 标准值 | 最小值 | 最小值 | 最小值 | 最小值 | 最小值 | 标准值 | 最小值 | 标准值 | ||
| N35 | 11.7 | 12.2 | 10.9 | 868 | ≥12 | ≥955 | 33 | 36 | 263 | 287 | ≤80 |
| N38 | 12.2 | 12.5 | 11.3 | 899 | ≥12 | ≥955 | 36 | 39 | 287 | 310 | ≤80 |
| N40 | 12.5 | 12.8 | 11.4 | 907 | ≥12 | ≥955 | 38 | 41 | 302 | 326 | ≤80 |
| N42 | 12.8 | 13.2 | 11.5 | 915 | ≥12 | ≥955 | 40 | 43 | 318 | 342 | ≤80 |
| N45 | 13.2 | 13.8 | 11.6 | 923 | ≥12 | ≥955 | 43 | 46 | 342 | 366 | ≤80 |
| N48 | 13.8 | 14.2 | 11.6 | 923 | ≥12 | ≥955 | 46 | 49 | 366 | 390 | ≤80 |
| N50 | 14 | 14.5 | 10 | 796 | ≥11 | ≥876 | 48 | 51 | 382 | 406 | ≤60 |
| N52 | 14.3 | 14.8 | 10 | 796 | ≥11 | ≥876 | 50 | 53 | 398 | 422 | ≤60 |
| N35M | 11.7 | 12.2 | 10.9 | 868 | ≥14 | ≥1114 | 33 | 36 | 263 | 287 | ≤100 |
| N38M | 12.2 | 12.5 | 11.3 | 899 | ≥14 | ≥1114 | 36 | 39 | 287 | 310 | ≤100 |
| N40M | 12.5 | 12.8 | 11.6 | 923 | ≥14 | ≥1114 | 38 | 41 | 302 | 326 | ≤100 |
| N42M | 12.8 | 13.2 | 12 | 955 | ≥14 | ≥1114 | 40 | 43 | 318 | 342 | ≤100 |
| N45M | 13.2 | 13.8 | 12.5 | 955 | ≥14 | ≥1114 | 43 | 46 | 342 | 366 | ≤100 |
| N48M | 13.6 | 14.3 | 12.9 | 1027 | ≥14 | ≥1114 | 46 | 49 | 366 | 390 | ≤100 |
| N35H | 11.7 | 12.2 | 10.9 | 868 | ≥17 | ≥1353 | 33 | 36 | 263 | 287 | ≤120 |
| N40H | 12.5 | 12.8 | 11.6 | 923 | ≥17 | ≥1353 | 38 | 41 | 302 | 326 | ≤120 |
| N42H | 12.8 | 13.2 | 12 | 955 | ≥17 | ≥1353 | 40 | 43 | 318 | 342 | ≤120 |
| N45H | 13 | 13.6 | 12.1 | 963 | ≥17 | ≥1353 | 43 | 46 | 326 | 358 | ≤120 |
| N48H | 13.7 | 14.3 | 12.5 | 955 | ≥17 | ≥1353 | 46 | 49 | 366 | 390 | ≤120 |
| N35SH | 11.7 | 12.2 | 11 | 876 | ≥20 | ≥1595 | 33 | 36 | 263 | 287 | ≤150 |
| N38SH | 12.2 | 12.6 | 11.4 | 907 | ≥20 | ≥1595 | 36 | 39 | 287 | 310 | ≤150 |
| N40SH | 12.6 | 12.9 | 11.8 | 939 | ≥20 | ≥1595 | 38 | 41 | 303 | 326 | ≤150 |
| N42SH | 12.9 | 13.2 | 12.4 | 987 | ≥20 | ≥1595 | 40 | 43 | 318 | 342 | ≤150 |
| N28UH | 10.2 | 10.8 | 9.6 | 764 | ≥25 | ≥1990 | 26 | 29 | 207 | 231 | ≤180 |
| N30UH | 10.8 | 11.3 | 10.2 | 912 | ≥25 | ≥1990 | 28 | 31 | 223 | 247 | ≤180 |
| N33UH | 11.3 | 11.7 | 10.7 | 852 | ≥25 | ≥1990 | 31 | 34 | 247 | 271 | ≤180 |
| N35UH | 11.8 | 12.2 | 10.8 | 860 | ≥25 | ≥1990 | 33 | 36 | 263 | 287 | ≤180 |
| N38UH | 12.2 | 12.5 | 11.3 | 899 | ≥25 | ≥1990 | 36 | 39 | 287 | 310 | ≤180 |
| N40UH | 12.5 | 12.8 | 11.3 | 899 | ≥25 | ≥1990 | 38 | 41 | 302 | 326 | ≤180 |
| N28EH | 10.4 | 10.9 | 9.8 | 780 | ≥30 | ≥2388 | 26 | 29 | 207 | 231 | ≤200 |
| N30EH | 10.8 | 11.3 | 10.2 | 812 | ≥30 | ≥2388 | 28 | 31 | 223 | 247 | ≤200 |
| N33EH | 11.3 | 11.7 | 10.5 | 836 | ≥30 | ≥2388 | 31 | 34 | 247 | 271 | ≤200 |
| N36EH | 11.7 | 12.1 | 10.8 | 860 | ≥30 | ≥2388 | 33 | 36 | 263 | 287 | ≤200 |
| 烧结钐钴产品特性 | ||||||||||
| Physical Properties of Sintered SmCo Magnets | ||||||||||
| 材料Material | 牌号 Grade | 剩磁Br | 矫顽力Hcb | 内禀矫顽力Hcj | 磁能积(BH)max | 工作温度 | ||||
| T | kA/m | kA/m | KJ/m3 | ℃ | ||||||
| Kgs | kOe | kOe | MGOe | |||||||
| Max | Min | Max | Min | Max | Min | Max | Min | |||
| SmCo5 and Sm(Pr)Co | XG18 | 0.92 | 0.82 | 756 | 639 | 1751 | 1194 | 159 | 127 | 250 |
| 9.2 | 8.2 | 9.5 | 8 | 22 | 15 | 20 | 16 | |||
| XG20 | 0.95 | 0.87 | 756 | 639 | 1751 | 1194 | 175 | 143 | ||
| 9.5 | 8.7 | 9.5 | 8 | 22 | 15 | 22 | 18 | |||
| XG22 | 1 | 0.93 | 772 | 660 | 1751 | 1194 | 191 | 159 | ||
| 10 | 9.3 | 9.7 | 8.3 | 22 | 15 | 24 | 20 | |||
| XG24 | 1.04 | 0.96 | 780 | 660 | 1751 | 1194 | 207 | 175 | ||
| 10.4 | 9.6 | 9.8 | 8.3 | 22 | 15 | 26 | 22 | |||
| Sm2Co17 | XGS24M | 1.04 | 0.96 | 772 | 318 | 955 | 398 | 207 | 175 | 350 |
| 10.4 | 9.6 | 9.7 | 4 | 12 | 5 | 26 | 22 | |||
| XGS24 | 1.04 | 0.96 | 780 | 660 | ≥1194 | 207 | 175 | |||
| 10.4 | 9.6 | 9.8 | 8.3 | ≥15.0 | 26 | 22 | ||||
| XGS24H | 1.04 | 0.96 | 780 | 660 | ≥1592 | 207 | 175 | |||
| 10.4 | 9.6 | 9.8 | 8.3 | ≥20.0 | 26 | 22 | ||||
| XGS26M | 1.07 | 1 | 796 | 318 | 955 | 398 | 223 | 191 | ||
| 10.7 | 10 | 10 | 4 | 12 | 5 | 28 | 25 | |||
| XGS26 | 1.07 | 1 | 820 | 677 | ≥1194 | 223 | 191 | |||
| 10.7 | 10 | 10.3 | 8.5 | ≥15.0 | 28 | 25 | ||||
| XGS26H | 1.07 | 1 | 820 | 677 | ≥1592 | 223 | 191 | |||
| 10.7 | 10 | 10.3 | 8.5 | ≥20.0 | 28 | 25 | ||||
| XGS28M | 1.1 | 1.04 | 796 | 318 | 955 | 398 | 239 | 207 | ||
| 11 | 10.4 | 10 | 4 | 12 | 5 | 30 | 26 | |||
| XGS28 | 1.1 | 1.04 | 820 | 677 | ≥1194 | 239 | 207 | |||
| 11 | 10.4 | 10.3 | 8.5 | ≥15.0 | 30 | 26 | ||||
| XGS28H | 1.1 | 1.04 | 820 | 677 | ≥1592 | 239 | 207 | |||
| 11 | 10.4 | 10.3 | 8.5 | ≥20.0 | 30 | 26 | ||||
| XGS30M | 1.12 | 1.07 | 796 | 318 | 955 | 398 | 247 | 223 | ||
| 11.2 | 10.7 | 10 | 4 | 12 | 5 | 31 | 28 | |||
| XGS30 | 1.12 | 1.07 | 820 | 677 | ≥1194 | 247 | 223 | |||
| 11.2 | 10.7 | 10.3 | 8.5 | ≥15.0 | 31 | 28 | ||||
| XGS32M | 1.15 | 1.09 | 796 | 318 | 955 | 398 | 262 | 238 | ||
| 11.5 | 10.9 | 10 | 4 | 12 | 5 | 32 | 29 | |||
| XGS32 | 1.15 | 1.09 | 820 | 677 | ≥955 | 262 | 238 | |||
| 11.5 | 10.9 | 10.3 | 8.5 | ≥12.0 | 32 | 29 | ||||
| 低温度系数 Low Temp.Coeff Sm2Co17 | XGL22LT | 1 | 0.93 | 756 | 677 | ≥1194 | 191 | 159 | 350 | |
| 10 | 9.3 | 9.5 | 8.5 | ≥15.0 | 24 | 20 | ||||
| XGL24LT | 1.04 | 0.96 | 756 | 677 | ≥1194 | 207 | 175 | |||
| 10.4 | 9.6 | 9.5 | 8.5 | ≥15.0 | 26 | 22 | ||||
| XGL26LT | 1.07 | 1 | 812 | 677 | ≥1433 | 223 | 191 | |||
| 10.7 | 10 | 10.2 | 8.5 | ≥18.0 | 28 | 25 | ||||
烧结汝铁硼产品性能参数表.pdf
烧结钐钴产品特性表.pdf